Can 310S Filler Wire Be Used to Weld 304L and 310S Stainless Steel?
Leave a message
Short Answer
Yes, 310S filler wire can be used to weld both 310S and 304L stainless steel. The filler is classified as ER310 under AWS A5.9, with a nominal 25 % chromium and 20 % nickel content, and it is a fully austenitic consumable. Whether that is the right engineering choice depends on the service: it is the correct and matched consumable for 310S base metal, and it is a workable but compromise solution on 304L where the benefits are high-temperature strength and the penalties are cost, hot-cracking sensitivity and lower pitting resistance in the deposit.
Chemistry of the Base Metals and the Filler
| Material | C, max | Cr | Ni | Mn, max | Si, max |
|---|---|---|---|---|---|
| 310S (UNS S31008) | 0.08 | 24.0 - 26.0 | 19.0 - 22.0 | 2.00 | 0.75 |
| 304L (UNS S30403) | 0.030 | 18.0 - 20.0 | 8.0 - 12.0 | 2.00 | 0.75 |
| ER310 wire (AWS A5.9) | 0.08 - 0.15 | 25.0 - 28.0 | 20.0 - 22.5 | 1.00 - 2.50 | 0.30 - 0.65 |
Two features of ER310 drive the welding behaviour. Its carbon range is higher than that of ER308L, and its chromium and nickel levels are far above those of 304L. When ER310 is deposited on 304L, dilution pulls the weld metal composition down towards roughly 20 % chromium and 15 % nickel in the first pass, so the final deposit sits between the two base metals rather than at either extreme.
Welding 310S to 310S
This is the matched joint and the reason the consumable exists. The 25Cr-20Ni deposit has the same high-temperature oxidation resistance and creep strength as the parent metal, which is why 310S piping and furnace parts are welded with ER310 wire or E310-16 covered electrodes (AWS A5.4). The weld is intended for service where metal temperatures are high enough that a 308L deposit would oxidise or creep too quickly. Because the deposit is fully austenitic, it contains no ferrite to resist solidification cracking, so a controlled heat input, stringer beads, a maximum interpass temperature and a clean joint preparation matter more here than on a 304L weld.
Welding 304L with 310S Filler
The joint is common in repair and mixed-fabrication work, where a 310S component must be joined to 304L pipe. Practical consequences are as follows. Strength at temperature improves, because the weld metal carries much more nickel and chromium than an ER308L deposit and retains strength when the 304L heat-affected zone begins to creep. Corrosion resistance in aqueous chloride service does not improve, because ER310 contains essentially no molybdenum and therefore has a pitting resistance equivalent number similar to or below that of 308L, far below 316L. Cost rises, because the consumable is more expensive than ER308L and welding speed is lower. Dilution makes the result variable, so the weld metal composition should be checked on the procedure qualification record rather than assumed. Where the joint will see chloride-bearing process fluid at temperature, ER316L or a nickel-based consumable is normally a better answer than ER310.
Welding Controls That Decide the Outcome
Qualify the procedure under ASME BPVC Section IX, with the joint configuration, filler classification, heat input range and interpass temperature recorded. Use TIG or MIG with argon shielding for manual work, or E310-16 electrodes for shielded metal arc welding, and keep the arc energy low with controlled weave. Purge and shield the root, cap the interpass temperature at a level that avoids carbide precipitation in the 304L heat-affected zone, and clean between passes. Post-weld heat treatment is not normally required for either joint, and solution annealing is impractical in the field, so the weld quality must come from procedure control. Where the finished joint will operate in the 425 to 815 degrees C range, remember that ER310 weld metal is the more stable of the two deposits while the 304L heat-affected zone remains the weak link in the joint.
Frequently Asked Questions
Q: Can ER310 filler wire be used to weld 304L?
A: Yes, it produces a sound joint with higher high-temperature strength than ER308L, but the deposit contains no molybdenum and offers no improvement in chloride pitting resistance.
Q: What is the AWS classification of 310S filler wire?
A: ER310 under AWS A5.9 for wire and rod, and E310-15 or E310-16 under AWS A5.4 for covered electrodes. The deposit nominally contains 25 % chromium and 20 % nickel.
Q: Why is 310S weld metal prone to cracking?
A: The deposit is fully austenitic and contains no ferrite to control low-melting phases during solidification, so it is more sensitive to solidification cracking and needs low heat input and controlled interpass temperature.
Q: Is post-weld heat treatment required after welding 304L with 310S filler?
A: No. The joint is normally left as-welded. Solution annealing, if specified, must be applied to the whole component and followed by rapid cooling.
Q: Which filler should be used for chloride service instead?
A: ER316L for aqueous chloride duty, or a nickel-based consumable for the most severe environments, because 310S weld metal contains no molybdenum.
Q: What service temperature suits a 310S-cored joint best?
A: Oxidising, high-temperature service in the 900 to 1100 degrees C band, where the 25Cr-20Ni deposit resists scaling and creep better than 18-8 weld metal.