Duplex stainless steels combine an austenitic matrix with roughly 40-50% ferrite, which gives about twice the yield strength of 304L or 316L together with far better resistance to chloride pitting and stress corrosion cracking. Duplex 2205, standardised as UNS S32205 with the older S31803 designation still widely ordered, is the volume grade of the family. Super duplex 2507, UNS S32750, is the higher-alloy member developed for seawater, subsea and high-chloride pressure duty. The two share the same metallurgical concept, so the choice is essentially a question of how much pitting and chloride stress corrosion resistance the project needs and whether the extra alloy content can be justified commercially.
Chemical Composition of 2205 and 2507
Both grades use nitrogen as an alloying element rather than a residual, which is what raises strength and pitting resistance at the same time. The table below gives the heat analysis ranges specified for plate, sheet and strip under ASTM A240/A240M, which is the usual purchasing document for duplex flat product. Pipe and tube are ordered to ASTM A790/A790M for seamless and welded duplex pipe, ASTM A928/A928M for electric-fusion-welded pipe, and ASTM A789/A789M for general-service duplex tubing.
| Element or Property | Duplex 2205 (S32205) | Duplex 2205 (S31803) | Super Duplex 2507 (S32750) |
|---|---|---|---|
| Carbon, max. | 0.030% | 0.030% | 0.030% |
| Chromium | 22.0-23.0% | 21.0-23.0% | 24.0-26.0% |
| Nickel | 4.5-6.5% | 4.5-6.5% | 6.0-8.0% |
| Molybdenum | 3.0-3.5% | 2.5-3.5% | 3.0-5.0% |
| Nitrogen | 0.14-0.20% | 0.08-0.20% | 0.24-0.32% |
| EN designation | 1.4462 X2CrNiMoN22-5-3 | 1.4462 | 1.4410 X2CrNiMoN25-7-4 |
Mechanical Properties Compared
Minimum room-temperature properties for annealed flat product to ASTM A240/A240M are shown below. Because the specification sets minimum values only, actual mill test results normally run above them; the important design point is that 2507 delivers roughly 20% more yield strength than 2205, which allows thinner wall thickness in pressure design.
| Property | Duplex 2205 (S32205) | Super Duplex 2507 (S32750) |
|---|---|---|
| Tensile strength, min. | 620 MPa | 795 MPa |
| Yield strength, min. | 450 MPa | 550 MPa |
| Elongation, min. | 25% | 15% |
| Hardness, max. | 30 HRC | 32 HRC |
| PREN | 34-36 | 40 and above |
The pitting resistance equivalent number follows PREN = %Cr + 3.3 x %Mo + 16 x %N. Applied to the specified ranges, 2205 lands near 34 while 2507 reaches about 41 at nominal composition, and this gap is the single best predictor of performance in chlorides.
Corrosion Performance and Service Limits
In ferric chloride pitting tests carried out to ASTM G48, 2507 consistently shows a higher critical pitting temperature than 2205, and its greater tolerance to chlorides also extends the chloride stress corrosion cracking threshold. 2205 remains the better economic choice for mildly chloride-bearing process streams, pulp and paper liquors and moderate-temperature heat exchangers. 2507 is normally selected for seawater systems, subsea manifolds, topside piping and high-pressure desalination duty. Both grades lose toughness if sigma phase forms, so long-term service is usually capped below about 300 °C, with published guidance for 2205 often quoted in the 250-300 °C band.
Fabrication, Welding and Heat Treatment
Duplex grades are solution annealed and then water or forced-air quenched; slow cooling in the 700-1000 °C region must be avoided because it precipitates sigma and secondary austenite. Stress relief is not practical once a component is complete, since the temperatures required would embrittle the material. Welding consumables are matched to the parent metal - typically a 2209 type filler for 2205 and a 2594 type filler for 2507 under AWS A5.9 - with controlled heat input, interpass temperature below about 150 °C and a nitrogen-bearing shielding gas to keep the ferrite-austenite balance in the weld pool. Machining behaviour is closer to a high-strength alloy steel than to 316L, and both grades work harden readily, so positive feeds and rigid tooling are essential.
Selection Guidance by Application
Choose 2205 for chemical process vessels, storage tanks, pulp mill digesters, flue gas desulphurisation equipment, and general heat exchanger tubing where chloride levels are moderate. Move to 2507 when the medium is seawater or brine at elevated temperature, when the design pressure calls for minimum wall thickness, or when chloride stress corrosion cracking of austenitic grades has already been recorded on similar service. In both cases, order to a duplex-specific specification rather than a generic stainless steel document, and confirm ferrite content and corrosion test results on the mill certificate.
Frequently Asked Questions
Q: Is super duplex 2507 magnetic?
A: Yes. The ferritic half of the microstructure makes 2507 clearly magnetic, roughly similar to 2205 and noticeably more magnetic than 304 or 316L, though not as strongly as a fully ferritic grade. This matters for magnetic particle inspection and for instrument components.
Q: What is 2507 equivalent to under other standards?
A: The grade is UNS S32750, EN 1.4410 / X2CrNiMoN25-7-4, and is covered by ASTM A240/A240M, A182/A182M, A790/A790M and A928/A928M for the common product forms. National designations vary, so the UNS number should always appear on the order.
Q: Is super duplex 2507 more expensive than 2205?
A: Yes, and the gap tracks the nickel, molybdenum and nitrogen content of the heat. The premium is normally in the range of one third to one half above 2205 for the same product form, and it widens when molybdenum prices rise.
Q: Can 2205 and 2507 be welded to each other?
A: They can, and a 2594 type filler is the usual conservative choice because it overmatches the weaker of the two parent metals. Dissimilar duplex joints should be qualified by procedure test, with ferrite content checked in the cap and root.
Q: What temperature limit applies to duplex stainless steel?
A: Both grades are generally limited to service below about 300 °C to avoid sigma phase formation and the associated loss of toughness and corrosion resistance. Short-term excursions above that level require assessment, and any fabrication that heats the material must be followed by a full solution anneal.
Q: How is duplex stainless steel identified on a mill certificate?
A: Look for the UNS number, the heat analysis including nitrogen, the specified minimum tensile and yield values, and the heat treatment condition. A ferrite content figure and, where specified, an ASTM G48 corrosion test result provide additional assurance of a correctly balanced microstructure.