Type 420 Stainless Steel: Martensitic Grade, Hardness and Applications
Leave a message
What 420 Stainless Steel Is
Type 420 is a martensitic stainless steel containing 12-14% chromium and a deliberate carbon content of 0.15-0.40%. Because it is martensitic rather than austenitic, it is ferromagnetic, it can be hardened by quenching, and it reaches useful hardness of about 50-55 HRC in thin sections after a low-temperature temper. That combination of hardness, edge retention and moderate corrosion resistance is why the grade dominates cutlery, valve trim, pump shafts and precision motion components.
The grade sits in the middle of the martensitic family. Type 410 with about 0.15% carbon is the general-purpose lower-carbon member, 420 raises carbon to gain hardness and wear resistance, and the high-carbon 440 grades push carbon towards 1% for bearings and cutting tools at the cost of corrosion resistance and weldability.
Equivalent Grades and Composition
| System | Designation |
|---|---|
| AISI / ASTM | Type 420, UNS S42000 |
| EN | 1.4021 / X20Cr13 |
| China | 20Cr13, historically written 2Cr13 |
| JIS | SUS420J1 and SUS420J2 |
| Element | Typical range |
|---|---|
| C | 0.15-0.40% |
| Cr | 12.0-14.0% |
| Mn | max 1.00% |
| Si | max 1.00% |
| P | max 0.040% |
| S | max 0.030% |
Steels in this family are supplied in the annealed condition at roughly 235 HBW maximum so that they can be machined, then hardened and tempered by the component manufacturer to the hardness the application needs.
Heat Treatment and Hardness
Annealing: 830-880 C, slow furnace cooling, to soften the structure for machining
Austenitising: 980-1060 C followed by oil quenching or air cooling in thin sections
Tempering: 150-370 C for maximum hardness of about 50-55 HRC, or 600-750 C for a tougher condition near 28-35 HRC
Stress relieving: 200-300 C below the tempering temperature where dimensional stability is critical
Tempering between roughly 400 C and 600 C should be avoided because it produces a marked drop in impact toughness without an offsetting gain in corrosion resistance. The correct selection depends on whether the part needs an edge, a shaft or a pressure-containing component, and the drawing should always state both hardness and the required toughness or impact value.
How Corrosion Resistance Actually Works
The corrosion resistance of any stainless steel comes from chromium held in solid solution. A continuous passive film requires at least about 10.5% chromium in the matrix, and the widely used n/8 rule describes the step change in passivity near 12.5%, or one eighth of the atomic ratio. Type 420 nominally contains 12-14% chromium, so its matrix is only just above the threshold in the as-quenched condition.
Carbon works against that margin. Each carbon atom consumes chromium as carbide, removing it from solid solution and creating chromium-depleted zones that become preferential sites for attack. This is why 420 must not be used for marine immersion, chloride-bearing process fluids or strong acids; it is chosen for mild service such as atmospheric exposure, fresh water, steam, food contact and mildly oxidising media. Free iron contamination from carbon-steel tooling, wire brushes or abrasive cloth is a separate and very common cause of surface rust spots, because the embedded iron corrodes even though the underlying steel is sound. Passivation in nitric or citric acid after grinding removes that contamination.
Corrosion and Quality Testing
Hardness testing to the applicable scale such as HRC or HRB, on a defined location of the part
Neutral salt spray exposure, or a boiling salt-water immersion test used for cutlery evaluation
Metallographic examination for retained austenite, carbide distribution and decarburisation
Dimensional and surface inspection, with the surface finish specified because a polished surface markedly improves corrosion behaviour
For any test of this type the result depends strongly on the surface condition. A specimen finished with a carbon-steel abrasive will show rust that has nothing to do with the alloy itself, so surface preparation must be documented together with the test method.
Fabrication Notes
Type 420 machines well in the annealed condition and is often supplied as ground bar for that reason. Welding is possible but demanding: preheating to about 200-300 C is required, a matching martensitic filler is used, and a post-weld temper at 700-750 C is needed to restore ductility in the heat-affected zone. Cracking risk rises sharply with carbon content and section thickness, so welded joints in 420 should be avoided where a 410 or an austenitic grade would do the job. Cold forming is limited by the high work-hardening rate, and stock should be annealed before any severe forming operation.
Where Type 420 Is Used
Knife blades, scissors and cutlery, surgical and dental instruments, valve stems, seats and trim, pump shafts and sleeves, moulds, plastic injection components, bushings, gauges and instrument parts, spindles and other precision machinery parts that need wear resistance together with moderate corrosion resistance. It is also used for household appliance components, fasteners and general hardware exposed to atmospheric and steam service.
Frequently Asked Questions
Q: Is 420 stainless steel magnetic?
Yes. It is martensitic, so it is ferromagnetic, unlike the austenitic 304 and 316 grades.
Q: What hardness can 420 reach?
About 50-55 HRC after austenitising near 1000 C, oil quenching and low-temperature tempering; a higher tempering temperature trades hardness for toughness and gives roughly 28-35 HRC.
Q: Is 420 stainless steel weldable?
It can be welded with preheat of about 200-300 C, a matching filler and a post-weld temper at 700-750 C, but the risk of cracking means it is avoided where another grade is acceptable.
Q: Is 420 suitable for marine or chloride service?
No. Its 12-14% chromium gives only moderate corrosion resistance, so it is used for atmospheric, fresh water, steam and mildly corrodent service, not for seawater or chloride-bearing process fluids.
Q: What is the difference between 410, 420 and 440C?
Type 410 contains about 0.15% carbon for general purpose use, 420 raises carbon to 0.15-0.40% for cutlery and wear parts, and the 440 grades approach 1% carbon for bearings and cutting tools.
Q: Why do polished 420 parts sometimes show rust spots?
Usually because free iron from carbon-steel tooling, brushes or abrasive cloth is embedded in the surface. Passivation in nitric or citric acid after finishing removes the contamination and restores the surface film.