SUS304, SUS304L, SUS316 and SUS316L Stainless Steel Bar Comparison
Leave a message
SUS304, SUS304L, SUS316 and SUS316L are the four austenitic grades from which most stainless bar stock is drawn for fasteners, shafts, valve trim, pump components and machined fittings. They share the same face-centred cubic structure and are all non-magnetic in the annealed condition after light working, but two variables separate them: carbon content, which controls behaviour after welding, and molybdenum content, which controls resistance to pitting and chloride attack. Understanding those two differences is enough to place the right grade on almost every drawing.
Standards That Apply to Stainless Bar
Bar is ordered under JIS G4303 for hot-rolled and JIS G4318 for cold-finished material when the SUS designation is used, or under ASTM A276/A276M and ASTM A479/A479M when the UNS designation applies, with ASTM A484/A484M covering general requirements such as tolerances, finish and marking. Fastener stock frequently adds ASTM A193/A193M or ASTM A320/A320M depending on temperature, and bar that will be machined into pressure parts is often dual certified so that a single heat satisfies both the Japanese and the American document.
Chemical Composition Compared
The table below gives the specified composition ranges. Carbon is the deciding factor between the standard and the L version of each grade, and molybdenum is the deciding factor between the 304 family and the 316 family.
| Element | SUS304 | SUS304L | SUS316 | SUS316L |
|---|---|---|---|---|
| Carbon, max. | 0.08% | 0.030% | 0.08% | 0.030% |
| Silicon, max. | 1.00% | 1.00% | 1.00% | 1.00% |
| Manganese, max. | 2.00% | 2.00% | 2.00% | 2.00% |
| Phosphorus, max. | 0.045% | 0.045% | 0.045% | 0.045% |
| Sulfur, max. | 0.030% | 0.030% | 0.030% | 0.030% |
| Chromium | 18.00-20.00% | 18.00-20.00% | 16.00-18.00% | 16.00-18.00% |
| Nickel | 8.00-10.50% | 9.00-13.00% | 10.00-14.00% | 12.00-15.00% |
| Molybdenum | - | - | 2.00-3.00% | 2.00-3.00% |
Mechanical Properties of Annealed Bar
Minimum values apply to the annealed condition, which is the normal supply condition for machined parts. Cold drawn or cold finished bar will be stronger in the direction of working, and that residual strengthening is not captured by the table, so a component that relies on it should be qualified by test rather than by specification.
| Property | SUS304 | SUS304L | SUS316 | SUS316L |
|---|---|---|---|---|
| Yield strength, min. | 205 MPa | 175 MPa | 205 MPa | 175 MPa |
| Tensile strength, min. | 520 MPa | 480 MPa | 520 MPa | 480 MPa |
| Elongation, min. | 40% | 40% | 40% | 40% |
| Hardness, max. | 187 HBW | 187 HBW | 187 HBW | 187 HBW |
Welding Behaviour and Intergranular Corrosion
When a standard carbon grade is heated in the range of roughly 450 to 850 °C, chromium carbides precipitate at the grain boundaries and the adjacent metal loses chromium. In a welded joint that zone lies next to the fusion line, and in a chloride or acidic medium it corrodes preferentially along the boundary. The L grades avoid the problem simply because there is not enough carbon available to form a continuous carbide network; they are the correct choice for tanks, reactors, pipe spools and any heavy section that will be welded without a post-weld solution anneal. Where a standard grade must be used in welded service, titanium or niobium stabilised variants are the alternative. A low-carbon grade is also easier to form into deep drawn or severely cold worked parts without an intermediate anneal.
Corrosion Resistance and Grade Selection
The 316 family contains molybdenum, which raises the pitting resistance equivalent number from about 18 for the 304 grades to about 24 for the molybdenum-bearing grades and shifts the tolerable chloride level upward. This is why marine hardware, chemical reactor internals and bleach-handling components use 316 or 316L rather than 304. Conversely, 304 remains perfectly adequate for architectural fittings, food machinery, general fasteners and indoor utility parts, and it is both cheaper and slightly stronger.
Selection checklist: use 304 where corrosion duty is mild and no welding is involved; use 304L where the part is welded and carbon pickup from the weld is a concern; use 316 where chlorides, pitting or crevice corrosion govern the design; use 316L where both chloride resistance and post-weld corrosion resistance are required. Machinability of all four grades is moderate, and the molybdenum-bearing grades are slightly tougher to cut, generating longer chips and requiring lower surface speeds. Free-machining variants with added sulfur or selenium exist for high-volume turned parts but have lower corrosion resistance and are not interchangeable.
Frequently Asked Questions
Q: Is SUS304 the same as 304 stainless steel?
A: Yes. SUS304 is the Japanese Industrial Standard designation and 304 is the AISI and UNS S30400 designation for the same grade. Composition limits and mechanical properties are essentially equivalent, though tolerances and marking requirements differ between documents.
Q: Should I always use the L grade instead of the standard grade?
A: No. The L grades are slightly weaker in the annealed condition and cost more, so they are justified mainly for welded or severely formed parts. For a machined component that is never welded, the standard grade performs equally well.
Q: Can 316L bar replace 304L bar directly?
A: In terms of strength and weldability the two are close, and 316L offers better chloride and pitting resistance. The main penalties are higher cost and slightly poorer machinability, so substitution is normally acceptable except where a drawing or code specifies the grade.
Q: Is stainless steel bar magnetic?
A: Annealed 304, 304L, 316 and 316L bar is essentially non-magnetic. Cold drawing, straightening and machining can induce a small amount of martensite and a slight magnetic response, which is normal and does not indicate a wrong grade.
Q: What surface conditions are available for stainless bar?
A: Common conditions are hot rolled and annealed, peeled and turned, cold drawn, ground and polished, with roughness and diameter tolerance chosen to suit the machining operation that follows. Bar destined for automatic turning is often supplied in the cold drawn or ground condition for dimensional consistency.
Q: How should the required grade be stated on a purchase order?
A: State the standard and edition, the grade designation including the UNS number, the product form and size, the condition, the surface finish and the required test certificates. Dual certification should be requested explicitly, since it requires the heat to meet the tighter of the two documents.